Is it necessary to holiday test the interior lining in the vapor phase (roof) of water storage tanks after coating?
Selected Answers
From
Josh Skinner of The Sherwin-Williams Company on
September 25, 2018:
Absolutely!!! Most interior roof spaces contain a ...read more
Absolutely!!! Most interior roof spaces contain a lot of irregular steel surfaces. The more edges, outside corners, crevices, welds, bolts you have, the greater your potential for holidays.
From
Bryant Chandler of Greenman-Pedersen, Inc. on
September 6, 2018:
Necessary, no. In most large tanks with roof rafte ...read more
Necessary, no. In most large tanks with roof rafters, the roof plates are not seal-welded to the rafters. The interface between the roof plate and the top flange of the rafters cannot be tested. Attempting to caulk the roof plate to rafter gap is expensive and has limited life, especially when maintenance personnel walk on the tank top, flexing the roof plates and breaking the caulking joint. On small tanks without rafters, then holiday testing has some merit if the owner wants to pay for it, considering access to the center of the roof for testing and touch-up can be expensive.
From
Larry Muzia of Exceletech Coating & Applications, LLC on
August 31, 2018:
Yes, Bill, it is I and hope you are well.
Best Re ...read more
Yes, Bill, it is I and hope you are well.
Best Regards
From
Bill Dollarhide of Individual on
August 29, 2018:
If the person who provided the answer is the same ...read more
If the person who provided the answer is the same Larry Muzia who once worked around Cape Canaveral many years back, then I, of course, agree with him, and also because we have re-blasted and coated a lot of undersides over the years.
From
Larry Muzia of Exceletech Coating & Applications, LLC on
August 28, 2018:
As there is more available oxygen above the liquid ...read more
As there is more available oxygen above the liquid, it is very important to have a pinhole-free lining, so my reply is Yes !