What type of generic coating is required to protect the inside of a tank containing liquid with pH ranging from 2 to 13 and operated at 65-80°C? Why?

More items for Coating Materials


Selected Answers

From William Slama of International Paint/Ceilcote Products on May 2, 2013:
     This is a correction to what I submitted previously First, it is important to realize that the pH range of 2-13 is generally considered moderate with regard to chemical aggressiveness to most polymers. For a pure acid solution, concentrations of about 0.1% sulfuric or hydrochloric acids would have that pH, although in buffered solutions, a higher concentration would be found to have that pH. Lime juice is about ph 2. Similarly, a pure alkaline solution of sodium hydroxide or potassium hydroxide would register pH of 2 at 1 to 2% concentration. So just knowing the pH alone doesn’t tell the story with regard to selecting a good lining. Some organic acids or other organics can be aggressive to polymers within that pH range. That being said, a vinyl ester or novolac vinyl ester or novolac epoxy system would probably withstand that range well. A bis A epoxy may even suffice. So, as said above, the pH range isn’t enough information for a confirmed lining recommendation. The other factor is, of course, the temperature. A singular issue with pH over 12 at temperatures over 120 F is the potential aggressiveness of the alkaline material to silica or silicatious filler content within the lining. In those cases, a barrier layer of the resin with a synthetic veil or carbon- or graphite-filled top (shield) coats are generally used. Independent of pH, for temperatures in that range, the lining must protect from water permeation in aqueous environments. For metallic substrates, a combination of external insulation and good permeation resistance of the film must be provided to avoid underfilm corrosion and subsequent blistering (cold wall effect). In many cases, large glass flake reinforcements are used to enhance permeation resistance. Concrete substrates are easier to protect in that regard since some water permeated through the lining will not cause corrosive degradation of the concrete, and permeated water can pass through the concrete porosity without much underfilm pressure buildup.

From William Slama of International Paint/Ceilcote Products on May 1, 2013:
     First, it is important to realize that the pH range of 2-13 is generally considered moderate with regard to chemical aggressiveness to most polymers. For a pure acid solution, concentrations of about 0.1% sulfuric or hydrochloric acids would have that pH, although in buffered solutions, a higher concentration would be found to have that pH. Lime juice is about ph 2. Similarly, a pure alkaline solution of sodium hydroxide or potassium hydroxide would register pH of 2 at 1 to 2% concentration. So just knowing the pH alone doesn’t tell the story with regard to selecting a good lining. Some organic acids or other organics can be aggressive to polymers within that pH range. That being said, a vinyl ester or novolac vinyl ester or novolac epoxy system would probably withstand that range well. A bis A epoxy may even suffice. So as said above, the pH range isn’t enough information for a confirmed lining recommendation. The other factor is, of course, the temperature. A singular issue with pH over 12 at temperatures over 120 F is the potential aggressiveness of the alkaline material to silica or silicatious filler content within the lining. In those cases a barrier layer of the resin with a synthetic veil of carbon- or graphite-filled top (shield) coats are generally used. Independent of pH, for temperatures in that range, the lining must protect from water permeation in aqueous environments. For metallic substrates, a combination of external insulation and good permeation resistance of the film must be provided to avoid underfilm corrosion and subsequent blistering (cold wall effect). In many cases large glass flake reinforcements are used to enhance permeation resistance. Concrete substrates are easier to protect in that regard since some water permeated through the lining will not cause corrosion.

From Per Gabrielsson of Free Lance Consultations and Inspections on May 1, 2013:
     APC say their MarineLine is perfect for that - but be careful! It does not come cheap - and why should it?!

From richard d souza of stoncor middle east llc on April 30, 2013:
     Use epoxy novolacs or novolac vinyl esters, but primers are required depending on whether the substrate is concrete or steel.

From Saulo Ventura of Ventura Coatings Technologies Inc. on April 29, 2013:
Novolac

Please sign in to submit your answer this question    

Tagged categories: Coating types; Coatings technology; Tank interiors


Current PSF Question | Submit a PSF Question | Full PSF Archive

Advertisements
 
Mitsubishi Gas Chemical America
 
Performance Amine 1,3-BAC
 
A highly reactive cycloaliphatic diamine offering superior performance. Reasonable cost and curing efficacy makes it suitable for all types of epoxy resin applications.
 

 
BASF
 
New resins from BASF will have metals loving water!
 
Excellent corrosion resistance, low VOC, high gloss, thin films www.basf.us/industrialcoatings dpsolutions@basf.com 800-231-7868
 

 
Tarps manufacturing, Inc.
 
QUALITY MADE IN AMERICA —Available near you!
 
CLICK to get a behind-the-scenes look at how Tarps Manufacturing makes the highest-quality tarps right here in the USA — available nationwide.
 

 
Industrial Vacuum Equipment Corp.
 
Hurricane Vacuums
& Dust Collectors
 
Vacuum and dust collector hose, filters and related accessories.
IndustrialVacuum.com
 

 
Carboline Company
 
Carboline launches new website!
 
The completely revamped website, offers quick and easy access to essential product information and is now mobile-friendly.
 

 
Jotun Paints Inc.
 
Jotun Jotachar 1709
 
Mesh-free passive fire protection epoxy designed to protect against hydrocarbon pool fire scenarios for up to four hours as defined in the ANSI/UL1709 standard.
 

 
SSPC: The Society for Protective Coatings
 
http://www.sspc.org/
 
Join SSPC and Enhance
Your Career !
 

 
Vector Technologies Ltd.
 
The Original Performance Proven Vacuum Solutions
 
VecLoader® 616 Double Dump, Continuous Vacuum, 170 HP w/ 2,400 CFM & 28” Hg. 33% More Efficient than traditional vacuum systems! Choose Vector for the most powerful and the most reliable trailer mounted vacuums in the industry! Email us at: inquiry@vector-vacuums.com or call us at: 800-832-4010
 

 
HoldTight Solutions Inc.
 
NO FLASH RUST - NO CONTAMINANTS
 
Our HoldTight®102 salt remover & flash rust
preventer prevents flash
rust by removing surface contaminants. Contact us
for your nearest distributor.
(800) 319.8802 sales@holdtight.com
 

 
Blastox/The TDJ Group, Inc.
 
Blastox® - One Step Lead Abatement
 
Sandblast additive delivered to jobsite pre-blended to eliminate hazardous abrasive wastes. Why mix, meter or apply at the job-site? Blast with ease and
Let your painters paint!
1(800)-252-7869
 

 
 
 

Technology Publishing Co., 1501 Reedsdale Street, Suite 2008, Pittsburgh, PA 15233

TEL 1-412-431-8300  • FAX  1-412-431-5428  •  EMAIL webmaster@paintsquare.com


The Technology Publishing Network

Durability + Design PaintSquare the Journal of Protective Coatings & Linings Paint BidTracker

 
EXPLORE:      JPCL   |   PaintSquare News   |   Interact   |   Buying Guides   |   Webinars   |   Resources   |   Classifieds
REGISTER AND SUBSCRIBE:      Free PaintSquare Registration   |   Subscribe to JPCL   |   Subscribe to PaintSquare News
MORE:      About PaintSquare.com   |   Privacy Policy   |   Terms & Conditions   |   Support   |   Site Map   |   Search   |   Contact Us